Grade contrast table: Stainless steel grade contrast | GB | JIS | AISI | DIN | 7Cr17 | SUS440A | 440A |
| 8Cr17 | SUS440B | 440B |
| 9Cr18, 9Cr18Mo | SUS440C | 440C |
|
Chemical composition table: Grade | composition (%) | C | Si | Mn | P | S | Cr | Mo | AISI440A | 0.60-0.75 | ≤1.00 | ≤1.00 | ≤0.040 | ≤0.03 | 16.0-18.0 | ≤0.75 | AISI440B | 0.75-0.95 | ≤1.00 | ≤1.00 | ≤0.040 | ≤0.03 | 16.0-18.0 | ≤0.75 | AISI440C | 0.95-1.20 | ≤1.00 | ≤1.00 | ≤0.040 | ≤0.03 | 16.0-18.0 | ≤0.75 |
AISI 440 mechnical property table: Heat treatment | σb MPa | σs MPa | σ5 % | ¢ % | HRC | ak 100 kJ/m2 | 1000~1050°C quenching in oil and 200~300°C tempering in oil or tempering in air | -- | -- | -- | -- | >58 |
| Annealing condition | 755 | -- | 14 | 27.5 | HB 230~240 | 1.57 |
|